| Productiopn Test Report |
| Test Description |
Standards |
Test Results |
Decision |
| Surface Abrasion |
>6000 |
6500 |
OK |
| |
>4000 |
/ |
/ |
| |
9000/AC4/ |
/ |
/ |
| |
4000/AC4/ |
/ |
/ |
| Modulus of Rupture |
>35N/mm2 |
37.6 |
OK |
| Internal Bond |
>1.2N/mm2 |
1.4 |
OK |
| Surface Soundess |
>1.0N/mm2 |
1.4 |
OK |
| Density |
>860kg/m3 |
900 |
OK |
| Swelling after 24 hours in water |
<12% |
9.7 |
OK |
| Moisture Content |
4%-7% |
5.9 |
OK |
| Resistance to Concentration of Acid on Overlay |
no Visible |
no visible |
OK |
| Resistance to Coldness & hotness cycle on surface |
'No cracks and blisters' |
no visible |
OK |
| Resistance to cigarette burns |
'No visible discoloration, cracks or blisters' |
no visible |
OK |
| Resistance to dry-hotness |
'No cracks and blisters' |
no visible |
OK |
| Anti-crack on surface |
0 / grade 0 |
Grade 0 |
OK |
| Resistance to Impact |
<9mm |
8.0 |
OK |
| Resistance to scratch |
>4.0N |
|
OK |
| Resistance to stain |
no visible |
no visible |
OK |
| FormaidehydeEmission |
Eo<0.5mg/L |
/ |
/ |
| |
E1<1.5mg/L |
0.6 |
OK |
| Anion Emission |
>800/cm3 |
/ |
/ |